![[Under Construction]](images/undercon.gif)



| |
MPIF Material Designations
-
| |
MPIF |
|
Density |
Tensile |
|
| Material |
Designation |
Chemistry |
(g/cc) |
(psi) |
Comments |
|
|
|
|
|
|
|
Iron |
F-0000 |
Pure Iron |
6.7 |
25,000 |
Soft magnetic material |
|
|
|
C < 0.03% |
|
|
|
|
|
|
|
|
|
|
Carbon Steel |
F-0008 |
0.8C |
6.9 |
54,000 |
Cost effective |
|
|
F-0008-HT |
|
|
85,000 |
|
|
|
|
|
|
|
|
Copper Steel |
FC-0208 |
2Cu, 0.8C |
6.7 |
60,000 |
Good sintered strength |
|
|
FC-0208-HT |
|
|
85,000 |
|
|
|
|
|
|
|
|
Nickel Steel |
FN-0205 |
2Ni, 0.5C |
7.1 |
57,000 |
Good heat-treated |
|
|
FN-0205-HT |
|
|
145,000 |
strength, impact energy |
|
|
|
|
|
|
|
Low-Alloy |
FL-4405 |
0.85Mo, 0.5C |
7.1 |
66,000 |
Good hardenability, |
|
Steel |
FL-4405-HT |
|
|
160,000 |
consistency in heat treatment |
|
|
|
|
|
|
|
Hybrid Low - |
FLN-4405 |
2Ni, 0.85Mo, 0.5C |
7.05 |
80,000 |
Best heat-treated |
|
Alloy Steel |
FLN-4405-HT |
|
|
170,000 |
strength, impact energy |
|
|
|
|
|
|
|
Diffusion - |
FD-0205 |
1.7Ni, 1.5Cu, 0.5Mo, 0.5C |
6.95 |
78,000 |
Best sintered strength |
|
Alloyed Steel |
FD-0205-HT |
|
|
130,000 |
|
|
|
|
|
|
|
|
Sinter - |
FLC-4608-HT |
1.75Ni, 1.5Cu, 0.5Mo, 0.8C |
7.0 |
100,000 |
Hardenability in sintering |
|
Hardened Steel |
|
|
|
|
|
|
|
|
|
|
|
|
Stainless Steel |
SS-316N2 |
17Cr, 12Ni, 2.5Mo |
6.5 |
60,000 |
Good corrosion resistance |
|
|
SS-430N2 |
17Cr |
7.1 |
60,000 |
and appearance |

|